Table 5. Average values and coefficient of variation for mechanical properties of 6-year-old Tectona grandis wood from thinning operations in Madre de Dios, Peru

Mechanical properties Average (6 yr) Max. Min. SD Coeff. var
Static bending
 EFLP (kg/cm2) 427.26 559.86 350.54 75.94 17.77
 MOR (kg/cm2) 562.19 668.72 482.10 74.00 13.16
 MOE (kg/cm2) 87,410.99 103,326.72 71,890.05 13,737.54 15.72
Parallel to the grain compression
 ELP (kg/cm2) 240.87 274.34 198.39 34.36 14.26
 RM (kg/cm2) 229.25 299.40 242.04 110.87 48.36
 MOE (kg/cm2) 1,471.60 2,098.70 788.60 526.14 35.75
Hardness
 Hardness at the ends (kg/cm2) 364.76 392.35 316.75 33.12 9.08
 Lateral or side hardness (kg/cm2) 372.00 436.20 298.99 56.27 15.13
 Parallel-to-grain shear (kg/cm2) 109.94 121.65 95.90 11.71 10.65
EFLP: fiber stress at the proportional limit, MOR: modulus of rupture, MOE: modulus of elasticity, RM: maximum resistance.