Table 3. Results of experimental studies of the production process of fiberboard with the addition of coniferous wood greenery
| Experiment number | The content of needles in the total mass, q, % | The size of the needle particles, f, mm | Board density, P, kg/m3 | Board strength, Pr, MPa | Board swelling in 24 hours, N, % | Water absorption of the board in 24 hours, S, % | Board thickness, T, mm | Moisture content of the board, W, % |
| 1 | 2 | 3 | 4 | 5 | 6 | 7 | 8 | 9 |
| 1 | 4 | 0.2 | 910 ± 2 | 41.6 ± 0.4 | 9.9 ± 0.1 | 20.0 ± 0.2 | 2.4 | 9.4 |
| 2 | 8 | 0.2 | 920 ± 2 | 42.2 ± 0.4 | 9.8 ± 0.1 | 20.1 ± 0.2 | 2.4 | 8.2 |
| 3 | 12 | 0.2 | 915 ± 2 | 39.8 ± 0.3 | 10.1 ± 0.1 | 21.2 ± 0.2 | 2.6 | 9.9 |
| 4 | 16 | 0.2 | 990 ± 3 | 28.2 ± 0.2 | 16.2 ± 0.2 | 26.7 ± 0.3 | 2.6 | 9.6 |
| 5 | 4 | 0.4 | 920 ± 2 | 37.2 ± 0.3 | 10.2 ± 0.1 | 20.6 ± 0.2 | 2.6 | 8.1 |
| 6 | 8 | 0.4 | 940 ± 2 | 39.8 ± 0.3 | 10.0 ± 0.1 | 20.7 ± 0.2 | 2.5 | 9.0 |
| 7 | 12 | 0.4 | 945 ± 2 | 34.5 ± 0.3 | 10.2 ± 0.1 | 21.9 ± 0.2 | 2.4 | 8.1 |
| 8 | 16 | 0.4 | 995 ± 3 | 28 ± 0.2 | 17.3 ± 0.2 | 27.9 ± 0.3 | 2.4 | 8.8 |
| 9 | 4 | 0.6 | 935 ± 2 | 36.2 ± 0.3 | 10.3 ± 0.1 | 20.9 ± 0.2 | 2.5 | 9.2 |
| 10 | 8 | 0.6 | 945 ± 2 | 39 ± 0.3 | 10.4 ± 0.1 | 21.2 ± 0.2 | 2.5 | 9.7 |
| 11 | 12 | 0.6 | 952 ± 2 | 37.5 ± 0.3 | 10.8 ± 0.1 | 22.8 ± 0.2 | 2.5 | 8.9 |
| 12 | 16 | 0.6 | 1,050 ± 3 | 27 ± 0.2 | 18.9 ± 0.2 | 29.3 ± 0.3 | 2.4 | 8.5 |
| 13 | 4 | 0.8 | 962 ± 2 | 35.6 ± 0.3 | 10.8 ± 0.1 | 21.6 ± 0.2 | 2.6 | 8.1 |
| 14 | 8 | 0.8 | 980 ± 2 | 37.9 ± 0.3 | 11 ± 0.1 | 22.3 ± 0.2 | 2.4 | 8.7 |
| 15 | 12 | 0.8 | 990 ± 3 | 36.1 ± 0.3 | 11.5 ± 0.1 | 23.8 ± 0.2 | 2.5 | 9.1 |
| 16 | 16 | 0.8 | 1,100 ± 4 | 25 ± 0.2 | 21.5 ± 0.2 | 32.5 ± 0.4 | 2.5 | 9.6 |
| Standard1) | - | - | 800–1,100 | °C 33 | ≤ 23 | - | 2.2–2.8 | ≤ 10 |
GOST 4598-86 Fiberboard for group B plates.