Table 3. The MOE and MOR values of samama wood under different treatments
| Treatments | Temperatures (°C) | Parameters |
| MOE (MPa) | MOR (MPa) |
| Untreated | - | 4,758.56 ± 670.23 | 59.40 ± 8.46 |
| Citric acid-impregnated | 140 | 5,054.47 ± 452.84 | 36.80 ± 8.73 |
| 160 | 4,742.37 ± 620.42 | 38.10 ± 8.97 |
| 180 | 4,574.62 ± 470.78 | 44.39 ± 7.38 |
| Heat-treated | 140 | 4,466.17 ± 623.54 | 49.41 ± 5.88 |
| 160 | 4,712.00 ± 793.95 | 52.87 ± 8.58 |
| 180 | 4,647.41 ± 565.29 | 56.91 ± 7.88 |
Those values are the average of 15 replications with standard deviation.