Table 4.
Color changes of the dyed regenerated-woody fiber with various concentration of commercial indigo dye

Concentration of Indigo (%, O.W.F.) λmax (nm) K/S Hunter's Value Munsell's Value

L* a* b* ΔE* H V C
Before After2) Before After2) Before After2)

0 450 0.73 76.05 5.21 22.18 0.2Y 0.6Y 7.52 6.68 3.45 5.27
1 650 0.43 69.49 -4.72 16.89 13.03 2.0GY 3.9Y 6.84 6.13 2.30 3.40
3 650 2.40 53.09 -8.66 2.09 33.52 9.4G 7.8GY 5.15 4.75 1.70 1.69
5 650 6.69 38.96 -6.84 -8.67 49.73 7.9B 3.9B 3.75 3.60 2.49 1.78
Dyeing conditions ; Temperature : 60 °C, Time : 60 minutes
After of 24hr ultraviolet irradiation treatment.