Table 2.
Chemical components of mengkuang pulp after LHW pretreatment.
| Temperature (°C) | Duration (minutes) | Alpha cellulose (%) | Hemicellulose (%) | Klason Lignin (%) | Acid Soluble Lignin (%) | Lignin Total (%) |
| Control | 0 | 77.89 | 10.32 | 9.79 | 2.01 | 11.80 |
| 140 | 20 | 67.60 | 9.59 | 7.70 | 0.67 | 8.37 |
| 30 | 73.32 | 9.06 | 6.67 | 1.29 | 7.96 |
| 40 | 66.23 | 9.25 | 7.08 | 0.77 | 7.85 |
| 160 | 20 | 68.97 | 8.96 | 7.76 | 0.69 | 8.45 |
| 30 | 77.45 | 9.93 | 6.32 | 1.50 | 7.82 |
| 40 | 67.45 | 9.93 | 8.01 | 0.75 | 8.76 |
| 180 | 20 | 67.23 | 5.90 | 7.94 | 0.63 | 8.57 |
| 30 | 76.24 | 9.77 | 6.65 | 1.08 | 7.73 |
| 40 | 62.40 | 7.02 | 8.27 | 0.72 | 8.99 |