Samples | Group | Weight percent gain/% | Mass loss/% | Durability class |
---|---|---|---|---|
Control | Control | 0 | 64.40±8.86 | Non durable |
CA treated wood | 0.3%C | 1.54±0.11 | 4.14±0.28 | Very durable |
0.5%C | 1.85±0.05 | 4.09±0.34 | ||
Paraffin emulsion treated wood | 0.5%W | 0.45±0.09 | 54.74±2.12 | Non durable |
2.0%W | 1.79±0.10 | 54.10±2.13 | ||
Compound system treated wood | 0.5%W/0.3%C | 1.32±0.06 | 2.88±0.14 | Very durable |
2.0%W/0.3%C | 3.30±0.17 | 5.16±0.43 | ||
0.5%W/0.5%C | 2.12±0.15 | 3.94±0.36 | ||
2.0%W/0.5%C | 3.79±0.04 | 4.49±0.33 |